material

SrHfO3

ID:

mp-3378

DOI:

10.17188/1206659


Tags: Strontium hafnate - LT Strontium hafnate

Material Details

Final Magnetic Moment
0.000 μB

Calculated total magnetic moment for the unit cell within the magnetic ordering provided (see below). Typically accurate to the second digit.

Magnetic Ordering
NM
Formation Energy / Atom
-3.813 eV

Calculated formation energy from the elements normalized to per atom in the unit cell.

Energy Above Hull / Atom
0.000 eV

The energy of decomposition of this material into the set of most stable materials at this chemical composition, in eV/atom. Stability is tested against all potential chemical combinations that result in the material's composition. For example, a Co2O3 structure would be tested for decomposition against other Co2O3 structures, against Co and O2 mixtures, and against CoO and O2 mixtures.

Density
7.51 g/cm3

The calculated bulk crystalline density, typically underestimated due calculated cell volumes overestimated on average by 3% (+/- 6%)

Decomposes To
Stable
Band Gap
4.177 eV

In general, band gaps computed with common exchange-correlation functionals such as the LDA and GGA are severely underestimated. Typically the disagreement is reported to be ~50% in the literature. Some internal testing by the Materials Project supports these statements; typically, we find that band gaps are underestimated by ~40%. We additionally find that several known insulators are predicted to be metallic.

Space Group

Hermann Mauguin
Pnma [62]
Hall
-P 2ac 2n
Point Group
mmm
Crystal System
orthorhombic

Electronic Structure

Topological data for ICSD ID 84280 from Topological Materials Database
Topological Classification
trivial*
Subclassification
LCEBR
* trivial insulator or metal
Linear Combination of Elementary Band Representations

Band Structure and Density of States

Warning! Semi-local DFT tends to severely underestimate bandgaps. Please see the wiki for more info.

X-Ray Diffraction

    Select radiation source:
  • Cu
  • Ag
  • Mo
  • Fe

Calculated powder diffraction pattern; note that peak spacings may be affected due to inaccuracies in calculated cell volume, which is typically overestimated on average by 3% (+/- 6%)

X-Ray Absorption Spectra

FEFF XANES

Select an element to display a spectrum averaged over all sites of that element in the structure.

Apply Gaussian smoothing:

0 eV
3 eV
FWHM: 0 eV

Download spectra for every symmetrically equivalent absorption site in the structure.

Download FEFF Input parameters.

Warning: These results are intended to be semi-quantitative in that corrections, such as edge shifts and Debye-Waller damping, have not been included.

Substrates

Reference for minimal coincident interface area (MCIA) and elastic energy:
substrate orientation:
substrate material substrate orientation film orientation elastic energy [meV] MCIA [Å2]
BN (mp-984) <0 0 1> <0 1 1> 0.006 175.3
GdScO3 (mp-5690) <1 0 1> <0 0 1> 0.008 169.2
LiGaO2 (mp-5854) <1 0 1> <1 1 0> 0.011 135.1
GaN (mp-804) <0 0 1> <0 1 1> 0.012 116.9
Si (mp-149) <1 0 0> <1 1 0> 0.014 270.2
SiO2 (mp-6930) <0 0 1> <0 1 1> 0.016 175.3
CeO2 (mp-20194) <1 0 0> <1 1 0> 0.017 270.2
InAs (mp-20305) <1 0 0> <0 0 1> 0.023 304.5
NdGaO3 (mp-3196) <1 1 0> <0 0 1> 0.025 304.5
LiAlO2 (mp-3427) <1 0 1> <1 1 1> 0.029 302.2
ZnTe (mp-2176) <1 0 0> <0 0 1> 0.032 304.5
LiAlO2 (mp-3427) <1 1 1> <1 1 0> 0.035 270.2
WSe2 (mp-1821) <1 1 1> <0 1 1> 0.044 175.3
TbScO3 (mp-31119) <0 0 1> <0 1 0> 0.050 95.3
GaSe (mp-1943) <0 0 1> <0 1 1> 0.055 175.3
Mg (mp-153) <1 1 1> <1 1 0> 0.066 270.2
ZrO2 (mp-2858) <1 0 1> <1 1 1> 0.066 302.2
CaCO3 (mp-3953) <0 0 1> <0 1 1> 0.067 175.3
MgAl2O4 (mp-3536) <1 1 0> <0 1 0> 0.068 95.3
CaCO3 (mp-3953) <1 0 0> <0 1 1> 0.069 175.3
GdScO3 (mp-5690) <0 0 1> <0 1 0> 0.071 95.3
WSe2 (mp-1821) <1 1 0> <0 1 1> 0.074 175.3
TbScO3 (mp-31119) <1 0 1> <0 0 1> 0.076 169.2
GaP (mp-2490) <1 0 0> <1 1 0> 0.079 270.2
LiF (mp-1138) <1 1 0> <0 1 0> 0.083 47.6
C (mp-66) <1 1 1> <0 1 1> 0.084 175.3
TeO2 (mp-2125) <1 0 1> <0 1 1> 0.088 233.7
WSe2 (mp-1821) <1 0 0> <1 1 1> 0.092 151.1
MgAl2O4 (mp-3536) <1 1 1> <0 1 1> 0.093 116.9
MgF2 (mp-1249) <1 0 1> <0 1 0> 0.101 238.2
Ga2O3 (mp-886) <1 0 -1> <0 0 1> 0.106 304.5
C (mp-66) <1 1 0> <0 1 0> 0.108 142.9
LiF (mp-1138) <1 1 1> <0 1 1> 0.109 58.4
C (mp-48) <1 1 1> <0 1 0> 0.112 238.2
MgAl2O4 (mp-3536) <1 0 0> <1 1 0> 0.114 67.6
LiAlO2 (mp-3427) <0 0 1> <1 1 0> 0.124 135.1
GaTe (mp-542812) <1 0 -1> <0 0 1> 0.124 304.5
TeO2 (mp-2125) <1 0 0> <0 1 0> 0.128 142.9
GaN (mp-804) <1 0 0> <0 1 0> 0.138 333.5
DyScO3 (mp-31120) <0 0 1> <0 1 0> 0.145 95.3
CaF2 (mp-2741) <1 0 0> <1 1 0> 0.147 270.2
AlN (mp-661) <0 0 1> <0 1 0> 0.153 238.2
MgO (mp-1265) <1 1 0> <0 1 0> 0.160 285.8
Ge (mp-32) <1 1 0> <0 1 0> 0.163 47.6
DyScO3 (mp-31120) <1 0 1> <0 0 1> 0.168 169.2
CdSe (mp-2691) <1 0 0> <0 0 1> 0.176 304.5
LiF (mp-1138) <1 0 0> <0 0 1> 0.179 33.8
CsI (mp-614603) <1 0 0> <0 0 1> 0.179 304.5
LaF3 (mp-905) <1 0 0> <0 0 1> 0.182 270.7
SiC (mp-7631) <0 0 1> <1 0 0> 0.197 335.3
Up to 50 entries displayed.
minimal coincident interface area.

Elasticity

Reference for tensor and properties:
Stiffness Tensor Cij (GPa)
272 85 109 0 0 0
85 288 96 0 0 0
109 96 271 0 0 0
0 0 0 88 0 0
0 0 0 0 94 0
0 0 0 0 0 93
Compliance Tensor Sij (10-12Pa-1)
4.5 -0.8 -1.5 0 0 -0.0
-0.8 4.1 -1.1 0 0 0.0
-1.5 -1.1 4.7 0 0 0.0
0 0 0 11.4 0 0
0 0 0 0 10.7 0
-0.0 0.0 0.0 0 0 10.8
Shear Modulus GV
91 GPa
Bulk Modulus KV
157 GPa
Shear Modulus GR
90 GPa
Bulk Modulus KR
157 GPa
Shear Modulus GVRH
91 GPa
Bulk Modulus KVRH
157 GPa
Elastic Anisotropy
0.03
Poisson's Ratio
0.26

Dielectric Properties

Reference for tensor and properties: Methodology
Dielectric Tensor εij (electronic contribution)
4.36 0.00 0.00
0.00 4.35 0.00
0.00 0.00 4.39
Dielectric Tensor εij (total)
34.75 0.00 0.00
0.00 33.59 0.00
0.00 0.00 29.66
Polycrystalline dielectric constant εpoly
(electronic contribution)
4.36
Polycrystalline dielectric constant εpoly
(total)
32.66
Refractive Index n
2.09
Potentially ferroelectric?
Unknown

Similar Structures beta feature

Explanation of dissimilarity measure: Documentation.
material dissimilarity Ehull # of elements
SmAlO3 (mp-7405) 0.1516 0.000 3
SrRuO3 (mp-22390) 0.0909 0.000 3
K3ClO (mp-572291) 0.1231 0.000 3
SrRuO3 (mp-557273) 0.0889 0.000 3
Sr3SiO (mp-30949) 0.0625 0.000 3
Sr2LuRuO6 (mp-20687) 0.1968 0.000 4
Sr2UNiO6 (mp-566457) 0.1768 0.099 4
Sr2UNiO6 (mp-645657) 0.1788 0.099 4
Sr2LuIrO6 (mp-22726) 0.1744 0.000 4
Sr2LuIrO6 (mp-561683) 0.1740 0.000 4
SrLaFeRuO6 (mp-697833) 0.2280 0.008 5
CaLaCrFeO6 (mvc-8975) 0.2274 0.028 5
CaLaMnFeO6 (mvc-16539) 0.2043 0.057 5
CaLaMnFeO6 (mp-40066) 0.2214 0.057 5
Up to 5 similar elemental, binary, ternary, quaternary, etc. structures displayed (dissimilarity threshold 0.75). Ehull: energy above hull per atom [eV].

Calculation Summary

Elasticity

Methodology

Structure Optimization

Run Type
GGA
Energy Cutoff
700 eV
# of K-points
None
U Values
--
Pseudopotentials
VASP PAW: Sr_sv Hf_pv O
Final Energy/Atom
-8.6989 eV
Corrected Energy
-182.2213 eV
Uncorrected energy = -173.9773 eV Composition-based energy adjustment (-0.687 eV/atom x 12.0 atoms) = -8.2440 eV Corrected energy = -182.2213 eV

Detailed input parameters and outputs for all calculations


Show JSON History Show BibTex Citation Download BibTex Citation
ICSD IDs
  • 184997
  • 161599
  • 162906
  • 164623
  • 89383
  • 86830
  • 162930
  • 187358
  • 84280
Submitted by
User remarks:
  • Strontium hafnate

Displaying lattice parameters for primitive cell; note that calculated cell volumes are typically overestimated on average by 3% (+/- 6%). Note the primitive cell may appear less symmetric than the conventional cell representation (see "Structure Type" selector below the 3d structure)