material

GdFeO3

ID:

mp-600862


Tags: Gadolinium iron(III) oxide Gadolinium ferrate(III) Gadolinium ferrate High pressure experimental phase Gadolinium iron trioxide

Material Details

Final Magnetic Moment
2.000 μB

Calculated total magnetic moment for the unit cell within the magnetic ordering provided (see below). Typically accurate to the second digit.

Magnetic Ordering
FiM
Formation Energy / Atom
-2.913 eV

Calculated formation energy from the elements normalized to per atom in the unit cell.

Energy Above Hull / Atom
0.000 eV

The energy of decomposition of this material into the set of most stable materials at this chemical composition, in eV/atom. Stability is tested against all potential chemical combinations that result in the material's composition. For example, a Co2O3 structure would be tested for decomposition against other Co2O3 structures, against Co and O2 mixtures, and against CoO and O2 mixtures.

Density
7.30 g/cm3

The calculated bulk crystalline density, typically underestimated due calculated cell volumes overestimated on average by 3% (+/- 6%)

Decomposes To
Stable
Band Gap
1.679 eV

In general, band gaps computed with common exchange-correlation functionals such as the LDA and GGA are severely underestimated. Typically the disagreement is reported to be ~50% in the literature. Some internal testing by the Materials Project supports these statements; typically, we find that band gaps are underestimated by ~40%. We additionally find that several known insulators are predicted to be metallic.

Space Group

Hermann Mauguin
Pnma [62]
Hall
-P 2ac 2n
Point Group
mmm
Crystal System
orthorhombic
We have not yet calculated a detailed bandstructure for this material

X-Ray Diffraction

    Select radiation source:
  • Cu
  • Ag
  • Mo
  • Fe

Calculated powder diffraction pattern; note that peak spacings may be affected due to inaccuracies in calculated cell volume, which is typically overestimated on average by 3% (+/- 6%)

X-Ray Absorption Spectra

FEFF XANES

Select an element to display a spectrum averaged over all sites of that element in the structure.

Apply Gaussian smoothing:

0 eV
3 eV
FWHM: 0 eV

Download spectra for every symmetrically equivalent absorption site in the structure.

Download FEFF Input parameters.

Warning: These results are intended to be semi-quantitative in that corrections, such as edge shifts and Debye-Waller damping, have not been included.

Substrates

Reference for minimal coincident interface area (MCIA) and elastic energy:
substrate orientation:
substrate material substrate orientation film orientation elastic energy [meV] MCIA [Å2]
GaP (mp-2490) <1 1 1> <0 1 0> 0.002 209.8
YAlO3 (mp-3792) <1 0 1> <0 0 1> 0.010 244.5
CaF2 (mp-2741) <1 1 1> <0 1 0> 0.016 209.8
SrTiO3 (mp-4651) <1 1 1> <0 1 1> 0.017 207.6
NdGaO3 (mp-3196) <1 1 0> <1 1 0> 0.018 60.8
TiO2 (mp-2657) <1 1 0> <0 1 1> 0.019 155.7
YVO4 (mp-19133) <1 0 1> <0 1 1> 0.025 207.6
KTaO3 (mp-3614) <1 1 0> <0 0 1> 0.025 91.7
NaCl (mp-22862) <1 1 0> <0 0 1> 0.025 91.7
AlN (mp-661) <0 0 1> <0 0 1> 0.027 152.8
InAs (mp-20305) <1 0 0> <1 1 0> 0.028 304.2
ZnTe (mp-2176) <1 0 0> <1 1 0> 0.035 304.2
Al (mp-134) <1 1 0> <0 0 1> 0.041 91.7
C (mp-48) <1 1 0> <1 0 0> 0.043 132.2
NdGaO3 (mp-3196) <1 1 1> <1 1 1> 0.044 68.1
MgF2 (mp-1249) <1 0 0> <1 1 1> 0.048 204.3
NdGaO3 (mp-3196) <1 0 0> <1 0 0> 0.052 44.1
ZrO2 (mp-2858) <0 1 0> <0 0 1> 0.053 305.7
BN (mp-984) <0 0 1> <0 0 1> 0.053 244.5
C (mp-48) <0 0 1> <0 0 1> 0.054 183.4
YAlO3 (mp-3792) <0 0 1> <0 1 0> 0.059 83.9
Ga2O3 (mp-886) <1 0 -1> <1 1 0> 0.062 304.2
SiC (mp-8062) <1 1 1> <0 1 0> 0.064 167.8
NdGaO3 (mp-3196) <1 0 1> <1 0 1> 0.068 53.6
TiO2 (mp-390) <1 1 0> <0 1 1> 0.073 51.9
TiO2 (mp-390) <0 0 1> <1 0 1> 0.076 214.5
AlN (mp-661) <1 0 1> <1 0 0> 0.078 88.1
TeO2 (mp-2125) <0 1 1> <0 0 1> 0.086 152.8
LaAlO3 (mp-2920) <1 0 1> <0 0 1> 0.086 152.8
MgF2 (mp-1249) <0 0 1> <1 0 1> 0.088 268.1
Si (mp-149) <1 1 1> <0 1 0> 0.093 209.8
Ni (mp-23) <1 0 0> <1 1 0> 0.094 60.8
Te2Mo (mp-602) <1 0 1> <0 1 0> 0.095 167.8
LiAlO2 (mp-3427) <0 0 1> <1 1 0> 0.098 243.4
CeO2 (mp-20194) <1 1 1> <0 1 0> 0.100 209.8
BN (mp-984) <1 1 1> <0 1 0> 0.101 167.8
InSb (mp-20012) <1 0 0> <1 0 1> 0.107 268.1
MgF2 (mp-1249) <1 0 1> <1 0 1> 0.110 53.6
MgO (mp-1265) <1 0 0> <1 1 0> 0.111 304.2
BaF2 (mp-1029) <1 1 0> <0 1 0> 0.114 167.8
TiO2 (mp-390) <1 0 1> <1 0 0> 0.117 352.5
LaF3 (mp-905) <1 0 1> <0 1 1> 0.119 207.6
CdTe (mp-406) <1 0 0> <1 0 1> 0.125 268.1
LiNbO3 (mp-3731) <0 0 1> <1 0 0> 0.137 308.4
LiGaO2 (mp-5854) <1 0 1> <1 1 0> 0.138 182.5
ZnO (mp-2133) <1 0 1> <1 0 0> 0.138 220.3
YAlO3 (mp-3792) <1 0 0> <0 0 1> 0.139 122.3
YVO4 (mp-19133) <1 0 0> <1 1 1> 0.144 136.2
CeO2 (mp-20194) <1 1 0> <0 1 0> 0.145 42.0
Si (mp-149) <1 1 0> <0 1 0> 0.149 42.0
Up to 50 entries displayed.
minimal coincident interface area.

Elasticity

Reference for tensor and properties:
Stiffness Tensor Cij (GPa)
141 26 69 0 0 0
26 235 73 0 0 0
69 73 240 0 0 0
0 0 0 74 0 0
0 0 0 0 55 0
0 0 0 0 0 79
Compliance Tensor Sij (10-12Pa-1)
8.2 -0.2 -2.3 0 0 0
-0.2 4.7 -1.4 0 0 0
-2.3 -1.4 5.3 0 0 0
0 0 0 13.4 0 0
0 0 0 0 18.2 0
0 0 0 0 0 12.7
Shear Modulus GV
71 GPa
Bulk Modulus KV
106 GPa
Shear Modulus GR
68 GPa
Bulk Modulus KR
96 GPa
Shear Modulus GVRH
70 GPa
Bulk Modulus KVRH
101 GPa
Elastic Anisotropy
0.38
Poisson's Ratio
0.22

Similar Structures beta feature

Explanation of dissimilarity measure: Documentation.
material dissimilarity Ehull # of elements
TbCrO3 (mp-769920) 0.0738 0.000 3
GdCrO3 (mp-19598) 0.0752 0.000 3
YCrO3 (mvc-10868) 0.0786 0.000 3
YCrO3 (mp-18725) 0.0787 0.000 3
GdVO3 (mp-615979) 0.0570 0.000 3
Sm2MgIrO6 (mp-980108) 0.1194 0.006 4
Ca2SnIrO6 (mvc-5666) 0.1298 0.067 4
Ca2SnSbO6 (mvc-3972) 0.1310 0.076 4
Y2MnNiO6 (mp-19192) 0.1876 0.000 4
Ca2CoIrO6 (mvc-5820) 0.1859 0.000 4
U2S3 (mp-672690) 0.6951 0.178 2
Fe3O4 (mp-715275) 0.6976 0.067 2
Al2O3 (mp-642363) 0.6192 0.279 2
Cr3C2 (mp-570112) 0.6412 0.030 2
Fe2O3 (mp-1078361) 0.6939 0.206 2
Mg11AlFeSi11O36 (mp-743592) 0.2922 0.206 5
LiLaNdSbO6 (mp-776091) 0.2818 0.006 5
LaMgCrSbO6 (mvc-9859) 0.3110 0.213 5
LaMgCrSnO6 (mvc-9925) 0.3179 0.138 5
CaLaMnRuO6 (mp-690556) 0.3080 0.000 5
Up to 5 similar elemental, binary, ternary, quaternary, etc. structures displayed (dissimilarity threshold 0.75). Ehull: energy above hull per atom [eV].

Calculation Summary

Elasticity

Methodology

Structure Optimization

Run Type
GGA+U
Energy Cutoff
520 eV
# of K-points
None
U Values
Fe: 5.3 eV
Pseudopotentials
VASP PAW: Gd Fe_pv O
Final Energy/Atom
-9.4178 eV
Corrected Energy
-207.7162 eV
-207.7162 eV = -188.3567 eV (uncorrected energy) - 10.9320 eV (MP Advanced Correction) - 8.4275 eV (MP Anion Correction)

Detailed input parameters and outputs for all calculations


Show JSON History Show BibTex Citation Download BibTex Citation
ICSD IDs
  • 27278
  • 150356
  • 150359
  • 150363
  • 150360
  • 16644
  • 150357
  • 23823
  • 189729
  • 172009
  • 150358
  • 150364
  • 150361
  • 247096
  • 61346
  • 150362
Submitted by
User remarks:
  • Gadolinium iron(III) oxide

Displaying lattice parameters for primitive cell; note that calculated cell volumes are typically overestimated on average by 3% (+/- 6%). Note the primitive cell may appear less symmetric than the conventional cell representation (see "Structure Type" selector below the 3d structure)