Final Magnetic Moment-0.000 μBCalculated total magnetic moment for the unit cell within the magnetic ordering provided (see below). Typically accurate to the second digit. |
Magnetic OrderingNon-magnetic |
Formation Energy / Atom-0.296 eVCalculated formation energy from the elements normalized to per atom in the unit cell. |
Energy Above Hull / Atom0.009 eVThe energy of decomposition of this material into the set of most stable materials at this chemical composition, in eV/atom. Stability is tested against all potential chemical combinations that result in the material's composition. For example, a Co2O3 structure would be tested for decomposition against other Co2O3 structures, against Co and O2 mixtures, and against CoO and O2 mixtures. |
Density8.75 g/cm3The calculated bulk crystalline density, typically underestimated due calculated cell volumes overestimated on average by 3% (+/- 6%) |
Decomposes ToMgIr + MgAg |
Band Gap0.000 eVIn general, band gaps computed with common exchange-correlation functionals such as the LDA and GGA are severely underestimated. Typically the disagreement is reported to be ~50% in the literature. Some internal testing by the Materials Project supports these statements; typically, we find that band gaps are underestimated by ~40%. We additionally find that several known insulators are predicted to be metallic. |
Hermann MauguinFm3m [225] |
Hall-F 4 2 3 |
Point Groupm3m |
Crystal Systemcubic |
sign indicates spin ↑ ↓
Calculated powder diffraction pattern; note that peak spacings may be affected due to inaccuracies in calculated cell volume, which is typically overestimated on average by 3% (+/- 6%)
substrate material | substrate orientation | film orientation | MCIA† [Å2] |
---|---|---|---|
C (mp-66) | <1 0 0> | <1 0 0> | 164.9 |
C (mp-66) | <1 1 1> | <1 1 1> | 285.7 |
GdScO3 (mp-5690) | <0 1 0> | <1 1 0> | 175.0 |
GdScO3 (mp-5690) | <1 1 0> | <1 0 0> | 329.9 |
Mg (mp-153) | <0 0 1> | <1 1 0> | 175.0 |
Mg (mp-153) | <1 0 0> | <1 0 0> | 206.2 |
LaF3 (mp-905) | <0 0 1> | <1 1 0> | 233.3 |
LaF3 (mp-905) | <1 0 0> | <1 0 0> | 206.2 |
PbS (mp-21276) | <1 0 0> | <1 0 0> | 329.9 |
GaP (mp-2490) | <1 1 0> | <1 1 0> | 175.0 |
GaP (mp-2490) | <1 1 1> | <1 1 1> | 214.3 |
InP (mp-20351) | <1 0 0> | <1 0 0> | 329.9 |
TbScO3 (mp-31119) | <0 1 0> | <1 1 0> | 175.0 |
TbScO3 (mp-31119) | <1 1 0> | <1 0 0> | 329.9 |
Ni (mp-23) | <1 0 0> | <1 0 0> | 206.2 |
Ni (mp-23) | <1 1 0> | <1 0 0> | 329.9 |
PbSe (mp-2201) | <1 0 0> | <1 0 0> | 329.9 |
BaTiO3 (mp-5986) | <0 0 1> | <1 0 0> | 82.5 |
NdGaO3 (mp-3196) | <0 1 0> | <1 1 0> | 175.0 |
NdGaO3 (mp-3196) | <1 0 0> | <1 1 0> | 175.0 |
SiC (mp-11714) | <1 0 1> | <1 0 0> | 288.7 |
MoSe2 (mp-1634) | <0 0 1> | <1 0 0> | 329.9 |
Ga2O3 (mp-886) | <1 0 -1> | <1 0 0> | 329.9 |
Ga2O3 (mp-886) | <1 0 0> | <1 0 0> | 164.9 |
Ga2O3 (mp-886) | <1 1 0> | <1 1 0> | 233.3 |
Si (mp-149) | <1 1 0> | <1 1 0> | 175.0 |
Si (mp-149) | <1 1 1> | <1 1 1> | 214.3 |
Au (mp-81) | <1 1 1> | <1 1 1> | 214.3 |
CdSe (mp-2691) | <1 0 0> | <1 0 0> | 329.9 |
WS2 (mp-224) | <0 0 1> | <1 1 0> | 175.0 |
C (mp-48) | <0 0 1> | <1 0 0> | 206.2 |
WSe2 (mp-1821) | <0 0 1> | <1 0 0> | 329.9 |
NaCl (mp-22862) | <1 0 0> | <1 0 0> | 164.9 |
NaCl (mp-22862) | <1 1 0> | <1 1 0> | 175.0 |
NaCl (mp-22862) | <1 1 1> | <1 1 1> | 214.3 |
Ge(Bi3O5)4 (mp-23352) | <1 0 0> | <1 0 0> | 206.2 |
CaCO3 (mp-3953) | <0 0 1> | <1 1 1> | 285.7 |
YAlO3 (mp-3792) | <0 1 0> | <1 1 0> | 116.6 |
YAlO3 (mp-3792) | <0 1 1> | <1 1 1> | 142.8 |
YAlO3 (mp-3792) | <1 0 1> | <1 1 1> | 142.8 |
Y3Fe5O12 (mp-19648) | <1 0 0> | <1 0 0> | 164.9 |
SiC (mp-8062) | <1 0 0> | <1 0 0> | 329.9 |
CdWO4 (mp-19387) | <0 0 1> | <1 1 1> | 285.7 |
CdWO4 (mp-19387) | <0 1 0> | <1 1 0> | 233.3 |
CdWO4 (mp-19387) | <1 0 0> | <1 1 1> | 285.7 |
CdWO4 (mp-19387) | <1 1 1> | <1 0 0> | 206.2 |
TiO2 (mp-390) | <1 0 1> | <1 1 0> | 116.6 |
CsI (mp-614603) | <1 1 0> | <1 1 0> | 175.0 |
MgF2 (mp-1249) | <0 0 1> | <1 0 0> | 206.2 |
MgF2 (mp-1249) | <1 0 0> | <1 0 0> | 247.4 |
Stiffness Tensor Cij (GPa) |
|||||
---|---|---|---|---|---|
110 | 96 | 96 | 0 | 0 | 0 |
96 | 110 | 96 | 0 | 0 | 0 |
96 | 96 | 110 | 0 | 0 | 0 |
0 | 0 | 0 | 67 | 0 | 0 |
0 | 0 | 0 | 0 | 67 | 0 |
0 | 0 | 0 | 0 | 0 | 67 |
Compliance Tensor Sij (10-12Pa-1) |
|||||
---|---|---|---|---|---|
48.1 | -22.4 | -22.4 | 0 | 0 | 0 |
-22.4 | 48.1 | -22.4 | 0 | 0 | 0 |
-22.4 | -22.4 | 48.1 | 0 | 0 | 0 |
0 | 0 | 0 | 14.9 | 0 | 0 |
0 | 0 | 0 | 0 | 14.9 | 0 |
0 | 0 | 0 | 0 | 0 | 14.9 |
Shear Modulus GV43 GPa |
Bulk Modulus KV100 GPa |
Shear Modulus GR15 GPa |
Bulk Modulus KR100 GPa |
Shear Modulus GVRH29 GPa |
Bulk Modulus KVRH100 GPa |
Elastic Anisotropy9.12 |
Poisson's Ratio0.37 |
material | dissimilarity | Ehull | # of elements |
---|---|---|---|
LiMgSnPd (mp-7555) | 0.0000 | 0.000 | 4 |
LiMgSbPt (mp-571584) | 0.0000 | 0.080 | 4 |
TiFeCoAs (mp-998974) | 0.0000 | 0.134 | 4 |
LiMgSbPd (mp-10179) | 0.0000 | 0.066 | 4 |
MnGaFeCo (mp-999552) | 0.0000 | 0.045 | 4 |
K3Sc (mp-973535) | 0.0000 | 0.607 | 2 |
V3Os (mp-866121) | 0.0000 | 0.000 | 2 |
V3Ru (mp-865382) | 0.0000 | 0.000 | 2 |
PrCd3 (mp-862755) | 0.0000 | 0.000 | 2 |
LiZn3 (mp-865907) | 0.0000 | 0.002 | 2 |
TiTc2Sb (mp-865809) | 0.0000 | 0.000 | 3 |
LiSbRh2 (mp-861667) | 0.0000 | 0.000 | 3 |
TbGaRh2 (mp-977421) | 0.0000 | 0.000 | 3 |
Ca2SbAu (mp-861950) | 0.0000 | 0.000 | 3 |
LiZn2Ni (mp-867252) | 0.0000 | 0.000 | 3 |
Be (mp-20) | 0.0000 | 0.083 | 1 |
Nb (mp-75) | 0.0000 | 0.000 | 1 |
Bi (mp-568610) | 0.0000 | 0.137 | 1 |
Br (mp-673171) | 0.0000 | 0.616 | 1 |
I (mp-684663) | 0.0000 | 0.455 | 1 |
Run TypeGGA |
Energy Cutoff520 eV |
# of K-points28 |
U Values-- |
PseudopotentialsVASP PAW: Mg_pv Ag Ir |
Final Energy/Atom-4.0178 eV |
Corrected Energy-16.0712 eV
-16.0712 eV = -16.0712 eV (uncorrected energy)
|
Displaying lattice parameters for primitive cell; note that calculated cell volumes are typically overestimated on average by 3% (+/- 6%). Note the primitive cell may appear less symmetric than the conventional cell representation (see "Structure Type" selector below the 3d structure)